Problems encountered in the printing of water-based plastic woven bags

1, back to stick

Phenomenon: After the plastic woven bag is printed, the ink layers stick to each other. Causes of failure: 1. After printing, there is a dry fake phase after printing. 2. The drying device is not in the right angle or fails. 3, because the printing speed is too fast, rewind too tight. 4, storage pressure is too large. 5, ink dilute penetration through India.

Remedy: 1, improve the ink drying speed. 2, increase the ventilation intensity check drying device angle. 3. Slow down the printing speed 4. When printing, stacking should be less or storage stacking load should be lighter. 5, adjust the ink viscosity or change another ink.

2, poor print fastness

Phenomenon: After the plastic woven bag is printed, the ink layer fades. Causes of failure: 1. PPPE surface corona is not handled well. 2, the printing shop temperature and relative humidity is too large. 3. The dissolved hydrogen bond strength of the ink system is too different from the hydrogen bond strength of the woven bag substrate.

Remedy: 1, woven bag substrate surface reaches 38 Dyne. 2, try to control the relative humidity of the workshop between 50-60%, but not too low, less than 40%, easy to generate static electricity. It is best to control the room temperature at 18-23 degrees, and keep the environment clean and air circulation. 3, ink selection should be very cautious (the same nature), the use of ink should be appropriate, as long as the viscosity is small and the ink system resin content is good.

3, shrinkage or elongation of the longitudinal pattern when printing or migrating printing

Failure reasons: 1, the ink is too thin (that is, the viscosity is too small). 2, paper or plastic substrates thin. 3, ink is too large. 4, printing pressure is too heavy. 5, filming is too slow.

Remedy: 1. Incorporate original ink or add thickener. 2, replace the compact substrate. 3, use a good dry ink or add volatile solvents. 4, adjust (reduce) the amount of ink supply. 5, printing pressure should be light.

4, blocked version

Failure reasons: 1, mainly the ink on the printing plate dry knot poor ink transfer. 2, mixed with plastic or paper scraps. 3, ink crust.

Remedy: 1, adjust the blowing angle (not directly on the printing plate). 2. In addition to changing the printing materials, the upper side of the printing machine should be separated from the fountain ink by the base paper, plastic or film. 3, replace the new ink

5, bleeding

Causes of failure: 1. Printed image edge seepage color (usually caused by the dye used in the ink). 2, using the wrong mix of pigments. 3. Excessive use of thinner materials, especially the poor solubility of thinner materials and inks.

Remedy: 1. Add oil to the ink or add a coupling agent. 2, replace the new ink. 3. Minimize the use of thinner materials, especially solvents that are compatible with the ink.

6, no ink film

Failure reasons: 1, poor gloss. 2, ink is rough. 3, ink drying too fast. 4, the ink system resin component is less or wrongly added matting agent.

Remedy: 1. Add the appropriate amount of ink in the ink. 2, re-grind or filter ink. 3, add water or original ink. 4, as little or as little add matting agents (such as wax, white carbon, etc.).

Custom Zipper

Custom Zipper

In today's word, more and more peope woul lie to add their own logo or text desgn on the produt. So as the ipper ndusty, many customer's requestsome appers with their own logo to show ther brand characteristc. Custom apper often made of four knds apper incude nyon ipper ny/on reverse zppe,refective zpper and waterproof ipper. Of course, sometimes one of the zipper can eamed ll of other three zippers' features. The lbgo prntng can beLase, Sublimated, Silk Screen Prnting and Jacquard to folow customer's design.The logo can also be design by us if customer aleady pace order.

Custom Zipper

Specification:

Size: 3# 4# 5# 8# 10#

Material: Nylon Teeth, Polyester or Cotton Tape

Color: Pantone, YCC, GCC, YKK

Slider: Reverse Auto Locking Slider

End Type: Close End or Open End

Feature: Hidden Teeth, with logo printed


We also have a special Transparent Zippers.

Transparent Zippers are one of the most Special Zipper branch, because it use PVC material as the Zipper tape that is big different from any other normal Zippers use polyester or cotton fabric. Zippers For Bags contained many different tape material: PVC, PP, PE, ABS, EVA and so on. And usually the color of Zipper For Bag is clear transparent, can also be change into other translucent or transparent color to suit customer's need. With features of good plasticity, low-priced and waterproof, PVC Zipper are widely used in garment, package, decoration and industry production.

Customized ZipperCustomize Zipper

Zipper For BagZipper Custom

Classification:

1. PVC Flat Zipper: The Zipper For Bags teeth top and bottom open or close with a metal or plastic puller
2. PVC Clip zipper: The PVC zipper teeth two side open or close with a clip puller
3. PVC Nylon Zipper: The PVC zipper tape sewed with nylon teeth
4. PVC Ziplock Zipper: Non Zipper Slider, and can be lock by itself.

Just ask for your customisation and we can make it for you!

Zipper Custom,Custom Zippers,Zipper For Bags,Zipper For Bag,Zippers For Bags

Shenzhen Yiyixing Zipper Manufacture Co.,Ltd , https://www.nicekeychain.com

Posted on